Optical Lithography Resources: Difference between revisions
Jump to navigation
Jump to search
| Line 21: | Line 21: | ||
| S1813 || Dehydrate on hot plate || 3000rpm || 1.5um || 115C 1min || X || - || - || X || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | | S1813 || Dehydrate on hot plate || 3000rpm || 1.5um || 115C 1min || X || - || - || X || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 (Link KNI recipe doc here) | ||
|- | |- | ||
| AZ5214 || Dehydrate on hot plate || | | AZ5214 || Dehydrate on hot plate || 3500rpm || 1.4um || 100C 1min || 25s || - || - || MF319 60s || - || Suss1 Ch1 15mW/cm^2 || Measured 10/19 | ||
|} | |} | ||
Revision as of 05:20, 4 November 2019
KNI Photoresists
Photoresists provided by KNI:
- S1813: standard positive, withstands acid etching. (Manufacturer Spec Sheet)
- AZ5214: positive and image reversal negative, good for liftoff. (Manufacturer Spec Sheet)
- SU-8: thick polymer structures. (Manufacturer Spec Sheet)
Positive Photoresist Recipes
See recipe notes for additional information on wafer cleaning and prep, edge bead removal, and spin curves.
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|
| S1813 | Dehydrate on hot plate | 3000rpm | 1.5um | 115C 1min | X | - | - | X | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 (Link KNI recipe doc here) |
| AZ5214 | Dehydrate on hot plate | 3500rpm | 1.4um | 100C 1min | 25s | - | - | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 |
Negative Photoresist Recipes
See recipe notes for additional information on wafer cleaning and prep, edge bead removal, and spin curves.
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|
| AZ5214 | Dehydrate on hot plate | 2000rpm | 1.8um | 100C 1min | 12s | 110C 1min | 40s | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 |
| Dehydrate on hot plate | 3500rpm | 1.4um | 100C 1min | 9s | 110C 1min | 30s | MF319 60s | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 |
SU-8 Recipes
SU-8 is available in thicknesses ranging from 500nm to 500microns. Remember to use Laurel Spinner 1.
Resist thicknesses currently provided by KNI: 2050, 2005, 2001, 2000.5
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|
| 2050 | Dehydrate on hot plate | 3000rpm | 50um | 65C 3min 95C 9min | X | 65C 2min 95C 7min | SU-8 Developer X seconds | Optional | Suss1 Ch1 15mW/cm^2 | Measured 10/19 |
Other Photoresists
Non-KNI Photoresist Recipes
| Resist | Wafer Prep | Spin | Thickness | Prebake | Exposure | Postbake | Flood | Development | Hardbake | Lamp | Notes |
|---|---|---|---|---|---|---|---|---|---|---|---|
| nLoF 2070 | Dehydrate on hot plate | 2500rpm | 7um | 110C 90s | 12s | 110C 90s | - | AZ 729 2min | - | Suss1 Ch1 15mW/cm^2 | Measured 10/19 |